Papworth’s Pty Ltd
Narngulu Synthetic Rutile
Plant
January 2004 Inspection
By F.Papworth Lyall Murphy
N
Pier 1
Pier 2
Drummy
Spalled
Spalled & drummy
Crack
Cold Joint
Panel Joint
Photo “Cooler
P2-11”
SR3 Cooler, Pier No 2
Photos
Figure 41
Photo “Cooler
P2-08”
Photo “Cooler
P2-01”
Photo “Cooler
P2-02”
Photo “Cooler
P2-10”
Photo “Cooler
P2-13”
Photo “Cooler P2-09”
Photo “Cooler P2-07”
Photo “Cooler P2-12”
Photo “Cooler
P2-03”
Photo “Cooler P2-06”
Photo “Cooler
P2-04”
“Cooler P2-05”
Services
ForPhoto
Engineers
& Contractors
Papworth’s Pty Ltd
Narngulu Synthetic Rutile
Plant
January 2004 Inspection
By F.Papworth Lyall Murphy
x
E
N
Q
G
I
A
F
J
B
H
K
C
L M
D
N O
P
Cover in mm, as measured with
cover meter
75mm diameter grinding core cut
Resistance for 4 probe Wenner
method with probes at 50mm
centres
630mm
Acid Leach Foundation
Detail 1 in Area A
Cover & Samples
Figure 5
590mm
Detail 1
=
=
=
ALF/S3
ALF/S2
ALF/S4
41mm x
41mm x
41mm x
42mm x
200mm
41mm x
40mm x
40mm x
40mm x
170mm
41mm x
40mm x
x
39mm x
160mm
1.29m
Detail 1
40mm
R=2520ohms
Vertical 25mm Ø bar cover = 40mm
Horizontal 12-15mm bar cover = 67mm
Depth of Carbonation = 0mm